Detailed Production Process of Aluminum Ingot Molds (Sand Casting Method)​

8KG Ingot Mold Front Photo

Step 1: Technical and Process Design​
This is the foundation of all subsequent work, determining the mold’s service life and the quality of the final aluminum ingots.

  • ​Customer Requirement Analysis:​​ Define the specifications of the aluminum ingots to be produced (e.g., weight, dimensions), expected production volume (mold lifespan requirements), and the casting line speed of the end-user.
  • ​Material Selection:​​ Choose the most suitable mold material based on requirements. ​Gray Iron (HT250/300)​​ offers low cost and wide application; ​Ductile Iron (QT500-7)​​ provides better strength, toughness, superior thermal fatigue resistance, and longer service life; for extremely demanding applications, ​heat-resistant alloy cast iron​ (e.g., with additions of Cr, Ni, etc.) is selected.
  • ​Structural Design:​​
    • ​Number of Cavities:​​ Designed as single or multiple cavities (common configurations: 4, 6, 8 cavities, etc.) to improve production efficiency.
    • ​Cooling System:​​ Design a rational cavity wall thickness and rib layout to ensure rapid and uniform solidification of the molten aluminum, which is critical for guaranteeing ingot quality and smooth demolding.
    • ​Gating System:​​ Design the pouring cup, sprue, runners, and ingates to ensure smooth metal flow and complete mold filling, avoiding defects like sand washing and gas porosity.
    • ​Other Features:​​ Design lifting lugs, mounting holes, locating pins, etc.

​Step 2: Pattern Making​

  • Based on the design drawings, create a ​wooden pattern​ (suited for small batch production or prototyping) or a ​metal pattern​ (typically aluminum, offering dimensional accuracy and durability, suited for mass production).
  • The pattern dimensions must be scaled up according to the ​shrinkage allowance​ of the cast iron (approximately 1% for iron).

​Step 3: Molding and Core Making​

  • ​Resin-bonded sand​ (e.g., Furan resin sand) is typically used for molding. This sand offers high strength, resulting in dimensionally accurate castings with a good surface finish.
  • ​Two-part (cope and drag)​​ or sometimes ​three-part molding​ is commonly employed. The pattern is placed in the flask, sand is filled and compacted around it, and then the pattern is removed, leaving the cavity.
  • The structure of an ingot mold is generally simple, usually ​not requiring separate sand cores.

​Step 4: Melting and Pouring​

  • Melt the iron in a ​medium-frequency induction furnace, with precise control over chemical composition and tap temperature (typically ≥1450°C).
  • ​Metallurgical Treatment before Pouring:​​ For gray iron, inoculation might be performed; for ductile iron, ​nodulizing (spheroidization) treatment and inoculation are essential.
  • Pour the qualified molten iron into the mold cavity. The pouring temperature is generally controlled between 1300-1380°C.

​Step 5: Shakeout and Cleaning​

  • After pouring, the casting is allowed to cool sufficiently within the mold (often for several hours, depending on weight and wall thickness) ​to prevent excessive internal stresses and the formation of chill (white iron)​.
  • After cooling, the casting is removed from the mold using a vibrating shakeout machine or manually.
  • The gating system (sprue, runners), risers, and flash are removed using cutting tools (e.g., torches, saws).

​Step 6: Heat Treatment​

  • ​Annealing​ is a critical step. Its purposes are:
    1. ​Stress Relieving:​​ To prevent distortion or cracking during subsequent machining or use.
    2. ​Reducing Hardness & Improving Machinability.​​
    3. ​Eliminating Chill Carbides (Ledeburite),​​ homogenizing the microstructure, and enhancing the mold’s thermal shock resistance.
  • ​Graphitizing Annealing​ is typically used, involving heating the castings to 850-950°C, holding at temperature, and then furnace cooling.

​Step 7: Machining​

  • After heat treatment, the casting is sent to the machine shop.
  • ​Rough Machining:​​ The base and mounting surfaces are milled or planed to ensure a flat reference plane.
  • ​Finish Machining:​​ ​CNC milling machines​ or ​machining centers​ are used for precision milling of the ​cavity working surfaces. This ensures dimensional accuracy and a high surface finish (typically requiring Ra ≤ 3.2 μm or better), which directly impacts the surface quality of the aluminum ingots.
  • Drilling lifting holes and connection holes.

​Step 8: Inspection and Trial Testing​

  • ​Dimensional Inspection:​​ Key dimensions are checked using calipers, depth gauges, and ​Coordinate Measuring Machines (CMM)​.
  • ​Visual Inspection:​​ Check for any casting defects (shrinkage, sand inclusions, cracks).
  • ​Trial Test (Optional but Highly Recommended):​​ New molds are sent to the customer’s facility or a test bench for actual pouring trials. This tests demolding performance, cooling efficiency, and the quality of the produced ingots, ensuring final validation.

​Step 9: Coating, Packaging, and Dispatch​

  • A ​refractory coating​ (e.g., graphite-based) is applied to the cavity working surfaces. This protects the mold surface, prevents molten aluminum from sticking, and aids release.
  • Apply anti-rust protection, package securely, and dispatch.

​Summary:​​ The production of aluminum ingot molds is a technically demanding, full-cycle casting process. It involves far more than simply casting; it integrates materials science, thermodynamics, mechanical design, and precision machining. The quality of the ingot mold directly determines the production efficiency and operating costs of the aluminum smelter.

0 replies